LSR Shrinkage and Dimensional Compensation: A Closed Loop from Trial to Production

Technical Articles
Article Sharing

Overview: Molding shrinkage for LSR is typically 2 to 4 percent, far higher than the 0.5 to 1.5 percent of a thermoplastic, and it shifts with mold temperature, cure time, wall thickness and compound hardness. Understanding how shrinkage behaves, and compensating for it accurately at the tooling stage, is the precondition for holding dimensional tolerance within plus or minus 0.05 mm.



Where Shrinkage Comes From


LSR shrinkage has two components: thermal shrinkage, the volume change on cooling from cure temperature to room temperature, which accounts for roughly 60 to 70 percent; and chemical shrinkage, the reduction in intermolecular spacing during crosslinking, at roughly 30 to 40 percent. That is a fundamental difference from a thermoplastic, which shrinks thermally and nothing else.


Ranked by weight, the influencing factors are: mold temperature, where every 20 degrees Celsius adds roughly 0.1 to 0.2 percent shrinkage; then cure time, where over-curing actually reduces post-shrinkage; then wall thickness, where thicker sections shrink more; then hardness, where softer compounds shrink more, 20 A running 0.5 to 1 percent above 70 A.


Weighting of factors affecting LSR shrinkage


Calculating the Compensation


The compensation formula for a cavity dimension is: cavity dimension = part dimension multiplied by (1 + shrinkage rate). In practice, though, the nominal shrinkage figure from the supplier cannot simply be applied — grade, running conditions and part geometry all introduce deviation.


The correct method is trial iteration: rough the first tool out at the nominal shrinkage figure, 2.5 percent say, then measure critical dimensions after the trial, calculate actual shrinkage and correct the cavity. Usually one or two rounds of correction converge on the target tolerance. To avoid repeated rework, critical dimensions can be left with allowance on the first round — cut the cavity slightly small and leave stock for finishing, rather than trying to hit final size in one go.


Trial iteration workflow for tool dimension compensation


Do Not Ignore Post-Shrinkage


A part is not stable the moment it leaves the tool. Left at room temperature for 24 to 72 hours it will shrink a further 0.1 to 0.3 percent, and if it goes through post-curing, 4 hours at 200 degrees Celsius, it will shrink another 0.2 to 0.5 percent. Leave this post-shrinkage out of the calculation and you get parts that measure in tolerance at demolding and come up small two days later.


So the timing of measurement has to be standardized: measure uniformly 24 hours after molding at normal temperature and humidity, and state it on the drawing. For parts with tight tolerances, post-curing can be specified before measurement, so post-shrinkage is built into the compensation.


How to Control Production


Once dimensions are stable and production starts, the control focus is process parameter stability: mold temperature within plus or minus 3 degrees Celsius, cure time within plus or minus 0.5 seconds, shot volume within plus or minus 1 percent. Drift in any of them shows up directly in dimensions.


On inspection, SPC is used: five parts sampled every two hours on critical dimensions, plotted on X-bar R control charts, with Cpk required at 1.33 or above. Any trend drift, seven consecutive points on one side, stops the machine for a check of mold temperature and the metering system. Zhongshan Henry Precision Technology Co., Ltd. (Henry Precision) runs a three-layer system on precision overmolding parts: full first-article dimensional inspection, SPC process control, and quarterly third-party re-measurement.


SPC dimensional control workflow for LSR production


Special Structures to Watch


Overmolded parts with metal inserts shrink in a more complicated way: the insert constrains the silicone, so shrinkage is low next to the insert and higher away from it, which easily produces warpage. The silicone layer should be kept as uniform in thickness as possible, avoiding locally thick sections.


Slender parts and thin-wall, large-flat parts are prone to warping. The answers are to optimize gate position for even filling, improve mold temperature uniformity, and where necessary add a sizing fixture — placing the part in a jig to cool after ejection.


Uneven shrinkage and warpage in insert overmolded parts

Table of Contents

Get Your Custom Liquid Silicone Overmolding Solution in 3 Steps

Get Your Custom Liquid Silicone Overmolding Solution in 3 Steps

Learn More

We use cookies to personalize and improve your browsing experience. By clicking "Accept All", you consent to our use of cookies.
You may read our Cookie Policy for details.

A Leader in Precision LSR Overmolding

A Leader in Precision LSR Overmolding

Professional Consultation Services
We patiently answer your questions and resolve your concerns
+86 189 2812 0729 (24/7)<br>+86 136 9169 4353 (Sales - Mr. Lu) +86 189 2812 0729 (24/7)
+86 136 9169 4353 (Sales - Mr. Lu)
sales@henry-precision.com sales@henry-precision.com
*Your Name
*Your phone
Your email
Company name
*Requirements
Country / Region
*Special Requirements

We use this information solely to contact you regarding potential cooperation.
By submitting, you agree to our Privacy Policy。

Rubber Coating Requirement Assessment

Please complete the following information so that we can provide you with the evaluation result.

*Your name
*Your phone
Upload the drawings

Size should not exceed 5M and support. Doc,.Docx,.Pdf

Yuanheng guarantees that the collection of your personal information is solely for the purpose of contacting you and helping you better understand us.
By sending this message, you are agreeing to our "Privacy Policy" and "Disclaimer".