1. Where Defects Come From


Defects in liquid silicone (LSR) precision overmolded parts fall mainly into four groups: bubbles, flash, sink marks and short shots. The causes are rarely simple — tooling design, process parameters, material condition and ambient conditions tend to interact. Bubbles, for instance, may come from poor venting, moisture in the material, or injection that is too fast. Flash relates directly to mold clearance and excessive injection pressure. Sink marks usually follow uneven cure or an abrupt change in wall thickness. A short shot can result from a blocked runner, insufficient injection pressure, or material that cured too early. Understanding the mechanism behind each defect, and how to trace it, is what protects production yield and holds quality cost down.


2. Bubbles and Burn Marks


Bubbles are among the most common defects in LSR parts, appearing as voids inside the part or on its surface. Three mechanisms account for most cases. Poor cavity venting: injection is fast, so if the vent groove at the parting line is too shallow, under 0.01 mm, or wrongly placed, air gets trapped in the compound. Moisture in the material: if the A or B component has been stored badly and picked up water, that water vaporizes at cure temperature and forms bubbles. Injecting too fast: high speed entrains air and folds it into the compound. Burn marks are the extreme case of the same phenomenon — trapped air compressed under high pressure spikes in temperature and carbonizes the silicone locally. The fixes follow from the causes: revise vent groove depth and placement, add vacuum-assisted venting, keep material storage humidity below 0.1 percent, and use a slow-fast-slow multi-stage injection profile to cut entrainment.


Close-up of bubbles and burn marks on a silicone part


Figure 1 Close-up of bubbles and burn marks on a silicone part


3. Flash


Flash is silicone squeezing out of the parting line, insert fits or ejector clearances and setting as a thin film. LSR's low viscosity, roughly 10 to 1,000 pascal-seconds, makes it extremely sensitive to clearance: once the parting line gap exceeds 0.01 mm, compound is driven into it under injection pressure and flash forms. The causes include tool wear or insufficient machining accuracy, excessive injection pressure, inadequate clamping force, and uneven mold temperature that locally opens the gap through expansion. Flash hurts appearance and assembly, and adds the cost of a deflashing operation. Fixes include tighter machining and clearance control, better matching of clamping force to injection pressure, regular inspection for tool wear, and cold runner gating designs that reduce the injection pressure peak.


Silicone flash along the mold parting line


Figure 2 Silicone flash along the mold parting line


4. Sink Marks and Short Shots


Sink marks show as depressions on the surface, usually over thick sections or behind ribs, where shrinkage during cure is not fed by material from outside. A short shot is an incompletely filled cavity, leaving the part locally missing or with an unfinished outline. For sink marks, the answers are to revise wall design and avoid abrupt thick sections, raise holding pressure and time, and lower mold temperature so the surface does not cure too early. Short shots take more digging: check the runner for blockage, particularly scorch residue in the cold runner; verify injection pressure and speed are sufficient; confirm the mix ratio, since A/B deviation changes viscosity; and check that mold temperature has not dropped far enough to hurt flow. Henry Precision works through first article inspection (FAI) and process capability analysis to find the root cause, then set corrective and preventive actions.


Good parts compared with sink mark and short shot defects


Figure 3 Good parts compared with sink mark and short shot defects


5. Henry Precision


Zhongshan Henry Precision Technology Co., Ltd. has built a complete defect analysis and quality improvement system for liquid silicone precision overmolding. With precision tooling, advanced inspection equipment and a deep process database, Henry Precision runs rapid root cause analysis and process optimization on bubbles, flash, sink marks and short shots alike, helping customers lift production yield to a stable, high level — treating precision as its foundation, and making sure every overmolded part is consistent in quality.

Table of Contents

Get Your Custom Liquid Silicone Overmolding Solution in 3 Steps

Get Your Custom Liquid Silicone Overmolding Solution in 3 Steps

Learn More

We use cookies to personalize and improve your browsing experience. By clicking "Accept All", you consent to our use of cookies.
You may read our Cookie Policy for details.

A Leader in Precision LSR Overmolding

A Leader in Precision LSR Overmolding

Professional Consultation Services
We patiently answer your questions and resolve your concerns
+86 189 2812 0729 (24/7)<br>+86 136 9169 4353 (Sales - Mr. Lu) +86 189 2812 0729 (24/7)
+86 136 9169 4353 (Sales - Mr. Lu)
sales@henry-precision.com sales@henry-precision.com
*Your Name
*Your phone
Your email
Company name
*Requirements
Country / Region
*Special Requirements

We use this information solely to contact you regarding potential cooperation.
By submitting, you agree to our Privacy Policy。

Rubber Coating Requirement Assessment

Please complete the following information so that we can provide you with the evaluation result.

*Your name
*Your phone
Upload the drawings

Size should not exceed 5M and support. Doc,.Docx,.Pdf

Yuanheng guarantees that the collection of your personal information is solely for the purpose of contacting you and helping you better understand us.
By sending this message, you are agreeing to our "Privacy Policy" and "Disclaimer".